SCR DeNOx: The Complete Guide
Direct answer: Selective Catalytic Reduction (SCR) removes NOx from flue gas by reacting it with ammonia over a V-Mo-Ti (vanadium-based) catalyst, converting NOx to nitrogen and water. It is the workhorse NOx control technology for coal power, steel, cement, glass and waste incineration — typically delivering 80–95% NOx removal within a defined temperature window. This guide is the hub: it summarizes the whole SCR topic and links to detailed articles on every part of it.
Key Engineering Point: SCR performance is set by the temperature window and the flue-gas condition at the catalyst face — dust, SO₂ and alkali metals degrade activity faster than age does. A catalyst chosen on removal rate alone fails if the inlet conditions are wrong.
Material entity profile
| Entity field | SCR DeNOx catalyst |
|---|---|
| Material class | Heterogeneous reduction catalyst |
| Composition | V₂O₅ (active) / MoO₃ or WO₃ (promoter) / TiO₂ (support); plate catalysts on steel mesh, honeycomb as extruded monolith |
| Structure | Macroporous monolith channels (pitch ~6–9 mm plate; 6–20 cells honeycomb) |
| Key properties | NOx conversion, SO₂→SO₃ oxidation rate, ammonia slip, pressure drop, erosion resistance |
| Target pollutants | NOx (NO + NO₂) |
| Mechanism | NH₃ + NOx → N₂ + H₂O over active sites |
| Regeneration | Chemical cleaning / rejuvenation in place or ex situ |
Data type: operating windows and design ranges are Typical Value engineering references; product data are Manufacturer Specification. See Data Classification and the Evidence Registry.
1. What SCR does and where it is used
SCR converts nitrogen oxides (NO and NO₂, together NOx) into harmless N₂ and water using ammonia as the reducing agent:
4NO + 4NH₃ + O₂ → 4N₂ + 6H₂O
The catalyst makes this reaction proceed at 200–420°C instead of the ~900°C that uncatalyzed thermal reduction would need. Applications:
| Industry | Typical duty |
|---|---|
| Coal-fired power | NOx compliance on high-dust flue gas |
| Steel & sintering | Sinter machine exhaust NOx |
| Cement | Kiln exhaust with high alkali dust |
| Glass & ceramics | High-temperature furnace NOx |
| Waste incineration | Municipal and hazardous waste flue gas |
| Chemical & refining | Tail gas and process vents |
2. How the catalyst works
The catalyst is titanium dioxide (TiO₂) support carrying vanadium pentoxide (V₂O₅) as the active component and tungsten or molybdenum trioxide (WO₃/MoO₃) as promoters that widen the temperature window and suppress SO₂ oxidation.
- Standard SCR: NO dominates; 4NO + 4NH₃ + O₂ → 4N₂ + 6H₂O.
- Fast SCR: NO₂ present accelerates the reaction at lower temperature.
- Side reaction to control: SO₂ oxidation to SO₃ (target ≤1%) and NH₃ oxidation at high temperature.
Ammonia is injected upstream — in coal power as anhydrous NH₃, aqueous ammonia or urea (decomposed to NH₃) — and mixed across the duct by an ammonia injection grid (AIG).
3. Catalyst types: plate vs honeycomb
Two geometries dominate. Details in Plate vs Honeycomb.
- Plate-type: metal mesh support with rolled catalyst paste — open channels, high erosion tolerance, the standard choice for high-dust coal flue gas.
- Honeycomb: extruded homogeneous catalyst — higher specific activity per volume, preferred where dust is moderate and volume is constrained.
Both are modular: elements are assembled into steel frames (modules) stacked in the reactor, typically 2+1 or 3+1 layers with a spare layer position.
4. Key design parameters
| Parameter | Typical range | Notes |
|---|---|---|
| Operating temperature | 200–420°C | Below window: low activity + bisulfate; above: NH₃ oxidation |
| Space velocity (SV) | 2,000–8,000 h⁻¹ | Depends on gas conditions and required conversion |
| Face velocity | 4–6 m/s | Balances pressure drop and erosion |
| Channel pitch | ~6–9 mm (plate), 6–20 cells (honeycomb) | Larger pitch for high dust |
| NH₃/NOx molar ratio | 0.8–1.05 | Above 1: rising ammonia slip |
| SO₂ oxidation rate | ≤1% | Formulation-dependent; SO₃ drives bisulfate issues |
| Design NOx removal | 80–95% | Set by permit and economic trade-off |
Data type: Typical Value engineering references for design guidance — not product specifications and not universal guarantees. Product-specific values are Manufacturer Specification; see Data Classification.
The selection decision path is covered step-by-step in the articles below — the short version: define gas conditions (temperature, NOx, SO₂, dust, moisture), choose geometry, size volume with deactivation margin, then verify with simulation testing on the actual gas.
5. Operation: the three watched numbers
SCR health is monitored through three trends, always together:
- NOx conversion at a fixed reference load and temperature.
- NH₃ slip — the early warning of active-site loss.
- Pressure drop — the signal for plugging and mechanical issues.
The details of controlling ammonia distribution, slip and flow conditioning are in Ammonia Slip Control.
6. Deactivation: how catalysts die
| Mode | Mechanism | Reversible? | Article |
|---|---|---|---|
| Arsenic poisoning | As₂O₃ vapor blocks pores | Mostly no | Poisoning |
| Alkali (K, Na) poisoning | Neutralizes acid sites | Partially (washing) | Poisoning |
| Ammonium bisulfate | SO₃ + NH₃ deposit below ~280–320°C | Yes (thermal/cleaning) | Poisoning |
| Ash plugging & erosion | Mechanical damage | Cleaning helps; erosion is terminal | Ash & Erosion |
| Thermal sintering | High-temperature structure loss | No | Replacement |
When performance falls, the decision between regeneration and replacement follows a measured sequence — Regeneration and Replacement cover both paths.
7. Performance verification
Catalyst activity is quantified as the activity K (m/h), derived from conversion at defined space velocity. Verification runs in three tiers: laboratory characterization, simulation with the real gas, and in-situ field testing — Activity Testing - Low-Temperature SCR — 160–250°C operation, ABS control, formulation choices. - Reactor Positioning — high-dust, low-dust and tail-end layouts. - Reducing Agent Systems — anhydrous ammonia, aqueous ammonia, urea. - Catalyst Volume Calculation — K, area velocity, layer management. - Flow Distribution & CFD - SNCR vs SCR — choosing the DeNOx route, hybrids, cost curves. - Cleaning & Maintenance — sootblowing, ΔP monitoring, inspection. — uniformity, AIG tuning, field verification..
8. Quick reference: symptom → cause
| Symptom | Most likely cause | Go to |
|---|---|---|
| Conversion falls, slip rises | Chemical deactivation | Poisoning |
| Conversion falls, ΔP rises | Plugging / ash | Ash & Erosion |
| Slip high, conversion fine | AIG imbalance or over-injection | Ammonia Slip |
| Performance falls after cleaning only slightly recovers | Irreversible poisoning | Regeneration |
| ΔP doubled since commissioning | Channel erosion/plugging | Replacement |
9. The complete SCR article series
- Plate vs Honeycomb SCR — geometry choice for dust, erosion and activity.
- SCR Catalyst Poisoning — arsenic, alkali metals, SO₂/SO₃ effects.
- SCR Regeneration — when washing works and when it doesn't.
- SCR Replacement — deciding when to change, sizing the replacement.
- Ammonia Slip Control — AIG tuning, distribution, stoichiometry.
- Ash, Erosion & Mechanical Life — pitch, face velocity, flow conditioning.
- Activity Testing — K value, lab/simulation/field verification.
When SCR is not the right choice
- Flue gas temperature far below the catalyst window with no reheating budget — evaluate SNCR, staging or a low-temperature formulation after a bisulfate audit.
- Very high SO₃ with no upstream control — catalyst poisoning and acid condensation dominate economics.
- Unknown fuel/poison profile with no test program — see Catalyst Selection for the full decision path.
- Space or pressure-drop constraints no catalyst geometry can satisfy.
10. Manufacturer perspective
SCR is a systems problem, not a catalyst purchase. The same NOx target can require 20–40% more catalyst volume on a high-poisoning fuel, and even the best catalyst behind a badly tuned AIG will slip ammonia from day one. We size from the current fuel and flue gas analysis, the measured velocity distribution and the outage window — and we recommend simulation testing with your actual gas before large orders.